Comparison of magnetic characteristics (JFE in-house data) : Rolling direction, shear cross-section
Material Thickness
(mm)
Specific resistance (mW-m) DC max
relative
permeability
Saturation
magnetiza-
tion (T)
Magnetic
flux density
B8(T)
Magnetic
flux density
B25(T)
Magneto- striction l10/400 (X10-6) Core loss (W/kg)
W10/50 W10/400 W10/1k W5/2k W2/5k W1/10k W0.5/20k
JNEX-Core 0.10 0.82 23.000 1.80 1.29 1.40 0.1 0.5 5.7 18.7 13.7 11.3 8.3 6.9
Grain-oriented silicon steel 0.23
0.35
0.48 92.000
94.000
2.03 1.92
1.92
1.96
1.96
-0.8 0.3
0.4
7.8
12.2
35.0
55.0
33.0
49.5
33.0
49.5
30.0
47.0
32.0
49.0
Non-oriented silicon steel 0.20
0.35
0.57 15.000
18.000
2.03
1.96
1.44
1.45
1.53
1.56
7.8 0.7
0.7
11.0
14.4
38.5
62.0
33.2
50.2
26.2
38.0
23.0
33.0
-
-
Fe-based amorphous 0.025 1.30 300.000 1.50 1.38 - 27.0 0.1 1.5 5.5 8.1 4.0 3.6 3.3
Ferrite Bulk - 3.500 - 0.37 - 21.0 - - - - 2.2 2.0 1.8

*W10/50 is the core loss at 50Hz, 1T(=10kG) when the magnetic flux sine wave is excited
*B8 is the magnetic flux density at 800A/m
*l10/400 is the magnetostviction at 400Hz, 1T when the magentic flux sine wave is excited.